Cement particles in water tend to cling together, trapping water inside the clusters. Sodium naphthalene formaldehyde (SNF) breaks up these clusters. This page explains how it works as a cement dispersant, what affects the result, and how to test it.
How SNF Disperses Cement
- Adsorption: the long anionic SNF molecules adsorb on the surfaces of cement grains and early hydration products.
- Charge: the sulfonate groups give the grains a strong negative surface charge (a more negative zeta potential).
- Repulsion: like-charged grains push each other apart, so clusters break up.
- Released water: water that was trapped in the clusters becomes free, so the paste flows more at the same water content.
Because the effect is electrostatic, it weakens as hydration products grow over the adsorbed layer. That is the reason for slump loss with SNF over time.
What Affects the Result
| Factor | Effect |
|---|---|
| Cement C3A and sulfate content | High-C3A cements adsorb more SNF, so more is needed |
| Time of addition | Adding after the cement is wetted often gives more flow from the same dose |
| Temperature | Faster hydration in heat means faster loss of flow |
| Sodium sulfate in the SNF | Part of the product weight; compare grades on active content |
| Other admixtures | Retarders and air entrainers can change the result |
Measuring Dispersion
- Cement paste fluidity (mini-slump spread): the SNF TDS specifies 220 mm min for SNF-5 and SNF-10, and 210 mm min for SNF-18 and SNF-20.
- Concrete slump or flow at the times you need.
- Water reduction at equal slump: the SNF-5 TDS reports 17% against a 14% minimum.
Where SNF Is Used as a Cement Dispersant
- Ready-mix and precast concrete.
- Dry-mix mortars, grouts and tile adhesives.
- Oil-well cement slurries.
- Gypsum and other mineral slurries.
Dose
The current TDS gives a supplier-recommended starting trial range of 0.5–1.0% powder by weight of cementitious material, with 0.75% as the first trial point. Confirm the working dose by trial mixes with your own cement, aggregates and admixtures.
Practical dosing steps are in how to use SNF in concrete. Specifications are on the SNF product page.
Frequently Asked Questions
How does SNF work as a cement dispersant?
It adsorbs on cement grains and gives them a negative charge, so they repel each other. Water trapped in clusters is released and the paste flows more.
Why does SNF lose effect over time?
Hydration products grow over the adsorbed SNF, reducing the repulsion. The loss is faster at higher temperature.
How is SNF dispersion measured?
With a cement paste fluidity (spread) test, and in concrete by slump and water reduction at equal slump.